Firing of lithium disilicate glass-ceramic (LS
2
)-supported restorations
Use the honey-combed firing tray and the corresponding support pins to fire the restorations.
Do not use ceramic pins, since they may stick to the restoration.
The processing temperatures must be observed. Increasing the firing temperature will result in severe vitrification
between the framework and the veneering ceramic, which may lead to crack formation later on. Reducing the firing
temperature results in the ceramic being underfired rendering it very brittle, which may ultimately lead to delamination.
The parameters in the Instructions for Use apply to Ivoclar Vivadent furnaces (tolerance: +/- 10 °C/18 °F)
If furnaces other than those from Ivoclar Vivadent are used, temperature adjustments may be necessary.
At the beginning, open the furnace and wait for the acoustic signal. Subsequently, place the firing tray with the objects
in the center of the firing table and start the program.
Remove IPS e.max objects from the furnace after completion of the firing cycle (wait for the acoustic signal of the
furnace).
Allow the objects to cool to room temperature in a place protected from draft.
Do not touch the hot objects with metal tongs.
Do not blast or quench the objects.
IPS e.max Ceram on B StÀ T H V1 V2
IPS e.max Press or IPS e.max CAD °C/°F min °C/°F/min °C/°F min °C/°F °C/°F
Staining technique
Stain and characterization firing
403/ 6:00 60/ 770/ 1:00 450/ 769/
757 6:00 108 1418 1:00 842 1416
Glaze firing
403/ 6:00 60/ 770/ 1:00 450/ 769/
757 6:00 108 1418 1:00 842 1416
Add-On after Glaze firing
403/ 6:00 50/ 700/ 1:00 450/ 699/
757 6:00 90 1292 1:00 842 1290
IPS e.max Ceram on B StÀ T H V1 V2
IPS e.max Press or IPS e.max CAD °C/°F min °C/°F/min °C/°F min °C/°F °C/°F
Cut-back and layering technique
Wash firing (foundation)
403/ 4:00 50/ 750/ 1:00 450/ 749/
757 4:00 90 1382 1:00 842 1380
Wash firing (foundation) characterization
403/ 4:00 50/ 750/ 1:00 450/ 749/
757 4:00 90 1382 1:00 842 1380
1
st
Dentin/Incisal firing
403/ 4:00 50/ 750/ 1:00 450/ 749/
757 4:00 90 1382 1:00 842 1380
2
nd
Dentin/Incisal firing
403/ 4:00 50/ 750/ 1:00 450/ 749/
757 4:00 90 1382 1:00 842 1380
Stain firing
403/ 6:00 60/ 725/ 1:00 450/ 724/
757 6:00 108 1337 1:00 842 1335
Glaze firing
403/ 6:00 60/ 725/ 1:00 450/ 724/
757 6:00 108 1337 1:00 842 1335
Add-On with Glaze firing
403/ 6:00 60/ 725/ 1:00 450/ 724/
757 6:00 108 1337 1:00 842 1335
Add-On after Glaze firing
403/ 6:00 50/ 700/ 1:00 450/ 699/
757 6:00 90 1292 1:00 842 1290
Depending on the furnace type, the firing temperature can be reduced by 5 °C to max. 10 °C (9 °F to max. 18 °F) for the
2
nd
Dentin / Incisal firing.
IPS e.max Ceram on IPS e.max Press or IPS e.max CAD (Cut-back and Layering technique)
IPS e.max Ceram on IPS e.max Press or IPS e.max CAD (Staining technique)
e.max
®
Ceram
Firing parameters