Depending on the furnace type, the firing temperature can be reduced by 5 °C to max. 10 °C (9 °F to max. 18 °F) for the
2
nd
Dentin / Incisal firing.
Firing of zirconium oxide (ZrO
2
)--supported restorations
Several units (e.g. multi-unit bridges with bulky pontics) in the furnace impede even and thorough heating of the
individual units.
Heat penetration in the firing chamber depends on the type of furnace and the size of the firing chamber.
The parameters listed in the Instructions for Use apply to Ivoclar Vivadent furnaces (temperature tolerance ± 10 ºC/18 °F).
If furnaces other than those from Ivoclar Vivadent are used, temperature adjustments may be necessary.
At the beginning, open the furnace and wait for the acoustic signal. Subsequently, place the firing tray with the objects
in the center of the firing table and start the program.
Remove IPS e.max objects from the furnace after completion of the firing cycle (wait for the acoustic signal of the
furnace).
Allow the objects to cool to room temperature in a place protected from draft.
Do not touch the hot objects with metal tongs.
Do not blast or quench the objects.
IPS e.max Ceram on IPS e.max ZirPress (Staining technique)
IPS e.max Ceram on IPS e.max ZirPress (Cut-back and Layering technique)
IPS e.max Ceram on IPS e.max ZirPress B StÀ T H V
1
V
2
L
Staining Technique °C/°F min °C/°F//min °C/°F min °C/°F °C/°F °C/°F
ZirLiner firing before wax-up and pressing 403/757 4:00 40/72 960/1760 1:00 450/842 959/1758
Stain and characterization firing 403/757 6:00 60/108 770/1418 1:00-2:00 450/842 769 450/842
Glaze firing 403/757 6:00 60/108 770/1418 1:00-2:00 450/842 769 450/842
Add-On after Glaze firing 403/757 6:00 50/90 700/1292 1:00 450/842 699 450/842
IPS e.max Ceram on IPS e.max ZirPress B StÀ T H V
1
V
2
L
Cut-back and Layering technique °C/°F min °C/°F/min °C/°F min °C/°F °C/°F °C/°F
ZirLiner firng before wax-up and pressing 403/757 4:00 40/72 960/1760 1:00 450/842 959/1758
Wash firing (Foundation) 403/757 4:00 40/72 750/1382 1:00 450/842 749/1380
Wash firing (Foundation) characterization 403/757 4:00 40/72 750/1382 1:00 450/842 749/1380
1
st
Dentin/Incisal firing 403/757 4:00 40/72 750/1382 1:00 450/842 749/1380
2
nd
Dentin/Incisal firing 403/757 4:00 40/72 750/1382 1:00 450/842 749/1380
Stain firing 403/757 6:00 60/108 725/1337 1:00 450/842 724/1335 450/842
Glaze firing 403/757 6:00 60/108 725/1337 1:00 450/842 724/1335 450/842
Add-On with Glaze firing 403/757 6:00 60/108 725/1337 1:00 450/842 724/1335 450/842
Add-On after Glaze firing 403/757 6:00 50/90 700/1292 1:00 450/842 699/1290 450/842